304 / 304L Stainless Steel Pipe and Tube: Chemistry, Strength and Standards

304 and 304L stainless steel pipe and tube chemistry, strength and standards

304 / 304L Stainless Steel Pipe and Tube: Chemistry, Strength and Standards

Will Lee - Account Manager, European Market at TeCarve
Will Lee
November 16, 2026
7 Min Read

304 stainless steel pipe and tube (UNS S30400, EN 1.4301) is the general-purpose 18 % chromium, 8–11 % nickel austenitic grade; 304L (S30403) limits carbon to 0.035 % for welded construction. In ASTM A312 pipe, TP304 requires at least 75 ksi [515 MPa] tensile and 30 ksi [205 MPa] yield strength, and TP304L at least 70 ksi [485 MPa] and 25 ksi [170 MPa]. This page collects the chemistry, strength, physical properties, equivalent designations and the ASTM pipe and tube standards that list 304, each from the standard named.

304 at a glance: UNS S30400 · EN 1.4301 · JIS SUS304 · density 7.9 g/cm³ · A312 TP304 min 515 MPa tensile / 205 MPa yield · melting range about 1,398–1,454 °C.

Chemical composition of 304, 304L and 304H pipe (ASTM A312)

Maximum values unless a range is shown, in weight percent, from ASTM A312/A312M-24b, Table 1.

GradeUNSC maxMn maxP maxS maxSi maxCrNi
TP304S304000.082.000.0450.0301.0018.0–20.08.0–11.0
TP304LS304030.035*2.000.0450.0301.0018.0–20.08.0–13.0
TP304HS304090.04–0.102.000.0450.0301.0018.0–20.08.0–11.0

* Footnote D to Table 1: for small diameter or thin walls or both, where many drawing passes are required, a carbon maximum of 0.040 % is necessary in grades TP304L and TP316L.

Mechanical properties (ASTM A312 minimums)

From ASTM A312/A312M-24b, Table 4. A312 publishes these values in ksi with MPa in brackets; the MPa figures are the standard’s own rounded values. Use the ksi to MPa converter for other figures.

GradeTensile strength, minYield strength, min
TP30475 ksi [515 MPa]30 ksi [205 MPa]
TP304L70 ksi [485 MPa]25 ksi [170 MPa]
TP304H75 ksi [515 MPa]30 ksi [205 MPa]

Equivalent designations

From EN 10088-1:2023, Table A.1, which rates these cross-references as comparable rather than identical grades. More grades are in the stainless steel grades chart.

System304304L
UNS (ASTM A959)S30400S30403
EN number / name1.4301 / X5CrNi18-101.4307 / X2CrNi18-9 (also 1.4306)
JISSUS304SUS304L
GB/T 20878S30408S30403

Physical properties

Guidance values from EN 10088-1:2023, Annex E (Table E.1) for steels 1.4301 and 1.4307; melting ranges from the SSINA Designer Handbook (Table 10) and the AK Steel 304/304L product data sheet. Details: stainless steel density, stainless steel melting point.

Property (20 °C)304 / 304L (EN 1.4301 / 1.4307)
Density7.9 g/cm³ (7,900 kg/m³)
Modulus of elasticity200 GPa
Mean thermal expansion, 20–100 °C16.0 × 10⁻⁶ /K
Thermal conductivity15 W/(m·K)
Specific heat capacity500 J/(kg·K)
Electrical resistivity0.73 Ω·mm²/m
Magnetizable (annealed)No
Melting range1,398–1,454 °C for 304 (SSINA); 1,399–1,454 °C for 304/304L (AK Steel)

EN 10088-1 notes that martensite formed by cold deformation, or small amounts of ferrite, increase the magnetizability of austenitic grades, so cold-worked or welded 304 can show slight magnetic response.

304 vs 304L vs 304H

  • 304: carbon up to 0.08 %; the standard choice where the pipe or tube is not welded extensively or is solution annealed after welding.
  • 304L: carbon up to 0.035 % in A312 (0.040 % for small or thin tube per footnote D); lower carbon reduces chromium carbide precipitation in weld heat-affected zones. Its minimum strength in A312 is lower than 304’s.
  • 304H: carbon controlled at 0.04–0.10 % for strength at elevated temperature, as used in boiler and superheater service.

304 contains no molybdenum, so in chloride-bearing water or atmospheres 316/316L is usually chosen instead; see 304 vs 316 vs 316L.

ASTM standards that list 304 pipe and tube

StandardProduct304 grades listed
ASTM A312/A312M-24bSeamless, welded and heavily cold-worked austenitic stainless steel pipeTP304, TP304L, TP304H
ASTM A213/A213M-24Seamless boiler, superheater and heat-exchanger tubes304, 304L (S30400, S30403)
ASTM A249/A249M-24aWelded boiler, superheater, heat-exchanger and condenser tubes304, 304L (S30400, S30403)
ASTM A269/A269M-25Seamless and welded austenitic stainless steel tubing for general service304, 304L (S30400, S30403)
ASTM A270/A270M-24Seamless and welded austenitic stainless steel sanitary tubing304, 304L (S30400, S30403)

Sizes and weights: stainless steel pipe schedule chart (ASME B36.19), stainless steel tube size chart and the stainless steel weight calculator. Pressure ratings: stainless steel pipe and tube pressure rating chart.

Written by Will Lee, Account Manager (Europe), TeCarve · Reviewed against ASTM / EN / ISO source documents · How we write and review our technical guides →
Will Lee - Account Manager, European Market at TeCarve

Author: Will Lee

Will Lee is TeCarve's Account Manager for Europe and the author of TeCarve's technical guides on stainless steel pipe and tube. His article on ASTM A312, A213 and A249 tubing was published in Stainless Steel World (October 2026). He reviews buyer specifications and drawings against ASTM, EN and DIN standards, advises on grade, tolerance and testing requirements, and checks the mill test certificates issued by the producing plants before European shipments.