409 Stainless Steel: Composition, Properties and 409 vs 304

409 stainless steel: ferritic titanium-stabilized grade, S40910, S40920 and S40930

409 Stainless Steel: Composition, Properties and 409 vs 304

Will Lee - Account Manager, European Market at TeCarve
Will Lee
November 18, 2026
6 Min Read

409 stainless steel (UNS S40900, EN 1.4512) is a titanium-stabilized ferritic stainless steel with 10.5–11.7 % chromium and almost no nickel (0.50 % max). It is magnetic, and its chromium is about half that of 304 (18.0–20.0 %). In ASTM A554 welded tube, S40900 has been replaced by three variants, S40910, S40920 and S40930, any of which may be supplied against an order for Type 409.

409 stainless steel chemical composition

Limits from ASTM A268/A268M-24 Table 1 (TP409) and ASTM A554-26 Table 1 (S40910, S40920, S40930); 304 from A554 Table 1 for comparison.

Element, %TP409 (S40900), ASTM A268S40910 / S40920 / S40930, ASTM A554304 (S30400) for comparison
Carbon, max0.080.0300.08
Manganese, max1.001.002.00
Phosphorus, max0.0450.0400.045
Sulfur, max0.0300.0200.030
Silicon, max1.001.000.75
Chromium10.5–11.710.5–11.718.0–20.0
Nickel0.50 max0.50 max8.0–11.0
Nitrogen, max–0.0300.10
Stabilizing elementsTi 6 × C min, 0.75 maxS40910: Ti 6 × (C+N) min, 0.50 max; Nb 0.17 max. S40920: Ti 8 × (C+N) min, Ti 0.15–0.50; Nb 0.10 max. S40930: (Ti+Nb) 0.08 + 8 × (C+N) min, 0.75 max; Ti 0.05 min–

S40900 vs S40910, S40920 and S40930

Footnote J to ASTM A554-26 Table 1 states that S40900 (Type 409) has been replaced by S40910, S40920 and S40930. Unless otherwise specified in the ordering information, an order for S40900 or Type 409 is satisfied by any one of the three at the option of the seller, and material meeting any of them may, at the manufacturer’s option, be certified as S40900. The three share the same base limits (0.030 % C max, 10.5–11.7 % Cr) and differ in how titanium and niobium are added to stabilize carbon and nitrogen. If a specific variant is required, name it on the order.

409 stainless steel mechanical properties (tube)

Property (ASTM A268 Tables 3 and 5)TP409 (S40900)
Tensile strength, min55 ksi (380 MPa)
Yield strength, min25 ksi (170 MPa)
Elongation in 2 in. (50 mm), min20 %
Hardness, max207 HB / 95 HRB

409 vs 304 stainless steel

409304
FamilyFerriticAustenitic
Chromium, %10.5–11.718.0–20.0
Nickel, %0.50 max8.0–11.0
Magnetizable (EN 10088-1 Annex E)Yes (1.4512)No (1.4301)
Mean thermal expansion 20–100 °C10.5 × 10⁻⁶/K16.0 × 10⁻⁶/K
Thermal conductivity at 20 °C25 W/(m·K)15 W/(m·K)
Density7.7 kg/dm³7.9 kg/dm³
Welded tube specificationASTM A554 (S40910, S40920, S40930), ASTM A268 (TP409)ASTM A554, A249, A269 and others

Physical properties of 409

EN 10088-1:2023 Annex E (1.4512, X2CrTi12; UNS S40900 per Table A.1): density 7.7 kg/dm³; modulus of elasticity 220 GPa at 20 °C; mean thermal expansion 10.5 (20–100 °C), 11.0 (20–200 °C), 11.5 (20–300 °C) and 12.0 × 10⁻⁶/K (20–400 °C and 20–500 °C); thermal conductivity 25 W/(m·K) and specific heat 460 J/(kg·K) at 20 °C; magnetizable.

Sources: ASTM A268/A268M-24, Tables 1, 3 and 5; ASTM A554-26, Table 1 and footnote J; EN 10088-1:2023, Annex E (Tables E.1 and E.3) and Table A.1.

Written by Will Lee, Account Manager (Europe), TeCarve · Reviewed against ASTM / EN / ISO source documents · How we write and review our technical guides →
Will Lee - Account Manager, European Market at TeCarve

Author: Will Lee

Will Lee is TeCarve's Account Manager for Europe and the author of TeCarve's technical guides on stainless steel pipe and tube. His article on ASTM A312, A213 and A249 tubing was published in Stainless Steel World (October 2026). He reviews buyer specifications and drawings against ASTM, EN and DIN standards, advises on grade, tolerance and testing requirements, and checks the mill test certificates issued by the producing plants before European shipments.