410 stainless steel (UNS S41000, EN 1.4006) is a martensitic straight-chromium stainless steel with 11.5–13.5 % chromium and up to 0.15 % carbon. Unlike 304 and 316 it contains no specified nickel, it is magnetic, and it can be hardened by heat treatment. For tube, it is listed as grade TP410 in ASTM A268, the specification for ferritic and martensitic stainless steel tubing.

410 stainless steel chemical composition

Limits for TP410 from ASTM A268/A268M-24 Table 1; 304 is shown from ASTM A554-26 Table 1 for comparison.

Element, %410 (TP410, S41000)304 (S30400) for comparison
Carbon, max0.150.08
Manganese, max1.002.00
Phosphorus, max0.0400.045
Sulfur, max0.0300.030
Silicon, max1.000.75
Chromium11.5–13.518.0–20.0
Nickelnot specified8.0–11.0

410 stainless steel mechanical properties (tube)

ASTM A268 tensile and hardness requirements for TP410 tube:

Property (ASTM A268 Tables 3 and 5)TP410 (S41000)
Tensile strength, min60 ksi (415 MPa)
Yield strength, min30 ksi (205 MPa)
Elongation in 2 in. (50 mm), min20 %
Hardness, max207 HB / 95 HRB

For tubing under 1/2 in. (12.7 mm) OD the elongation values for strip specimens in A268 Table 4 apply, and mechanical property requirements do not apply to tubing under 1/8 in. (3.2 mm) OD or with walls under 0.015 in. (0.4 mm).

Physical properties of 410

Property (EN 10088-1 Annex E, 1.4006)410
Density7.7 kg/dm³
Modulus of elasticity at 20 °C215 GPa
Mean thermal expansion 20–100 °C / 20–400 °C10.5 / 12.0 × 10⁻⁶/K
Thermal conductivity at 20 °C30 W/(m·K)
Specific heat at 20 °C460 J/(kg·K)
MagnetizableYes

Compared with 304 (EN 1.4301: 16.0 × 10⁻⁶/K and 15 W/(m·K)), 410 expands less and conducts heat about twice as well. Values at other temperatures are in stainless steel thermal expansion and conductivity by grade.

Heat treatment and hardening

  • Hardenable: ASTM A268 (1.1) notes that TP410 and UNS S41500 are amenable to hardening by heat treatment, and that this should be recognized in their use.
  • Tube as delivered: A268 (7.1) requires a final heat treatment in which the tubes are reheated to 1200 °F (650 °C) or higher and cooled, as appropriate for the grade, to meet the requirements of the specification, including the 207 HB maximum hardness of Table 5.
  • Magnetic: A268 describes its straight-chromium grades as ferromagnetic, and EN 10088-1 lists 1.4006 as magnetizable; see is stainless steel magnetic.

Which tube specification covers 410

  • ASTM A268: seamless and welded ferritic and martensitic stainless steel tubing for general corrosion-resisting and high-temperature service, grade TP410.
  • ASTM A554 (welded mechanical tube) does not list 410; the related grade it lists is 410S (S41008), with 0.08 % carbon max and 11.5–13.5 % chromium. See the ASTM A554 guide.
  • Equivalents: EN 1.4006 (X12Cr13), JIS SUS410, per EN 10088-1 Table A.1. More grades are in the stainless steel grades chart.

Sources: ASTM A268/A268M-24, sections 1 and 7, Tables 1, 3 and 5; ASTM A554-26, Table 1; EN 10088-1:2023, Annex E (Table E.4) and Table A.1.

Written by Will Lee, Account Manager (Europe), TeCarve · Reviewed against ASTM / EN / ISO source documents · How we write and review our technical guides →
Will Lee - Account Manager, European Market at TeCarve

Author: Will Lee

Will Lee is TeCarve's Account Manager for Europe and the author of TeCarve's technical guides on stainless steel pipe and tube. His article on ASTM A312, A213 and A249 tubing was published in Stainless Steel World (October 2026). He reviews buyer specifications and drawings against ASTM, EN and DIN standards, advises on grade, tolerance and testing requirements, and checks the mill test certificates issued by the producing plants before European shipments.